Four UV Adhesive Chemistries and the Job Each One Does

Editorial responsibility for this article rests with Wuhan Ooi Photoelectric Technology Co., Ltd. Written and reviewed by the Ooitech editorial team. See our editorial policy for how we write, where AI tools are used, and how to request a correction.

Four UV Adhesive Chemistries and the Job Each One Does

Quick answer: Four chemistries, two job descriptions. In a 0BB module a UV adhesive pins the ribbon onto fingers only 20 to 30 µm wide, so it has to cure in seconds, stay tough through thermal cycling, and not yellow in daylight. In a BC module something has to sit between a ribbon and the opposite-polarity fingers it crosses, so that layer has to be hard, pinhole-free, and still insulating after damp heat. Acrylate cures fastest, adjusts over the widest range and costs least, which is why positioning adhesives are usually built on it. Cationic epoxy shrinks little, has no oxygen problem at the surface, insulates well, and is the usual direction for the insulating layer, alone or inside a hybrid. The two hybrids buy one property each: speed with hardness, or toughness against the copper-to-silicon expansion gap. Read the job first, then the shadow the lamp cannot reach, then yellowing and insulation. Cost last.

These two products are discussed as if the words named one material. They do not. A positioning adhesive and an insulating adhesive sit in the same module, under the same lamp, and are asked for opposite properties. That is why four chemistries are in production.

Two new jobs, one new material

In an MBB or SMBB string the solder joint is the fixture: the ribbon is welded onto busbar pads, and once that joint cools the ribbon is not going anywhere. Remove the busbar and the pad goes with it. The ribbon now lands on fingers 20 to 30 µm wide and has to be held there before the string can be lifted. That is the positioning adhesive, also called the fixing or ribbon bonding adhesive, and the structure it answers to is the subject of what removing the busbar changes.

BC adds a second job with a different purpose. Both polarities of finger sit on the rear, alternating, and each ribbon contacts one polarity only. Every place a ribbon crosses a finger of the opposite polarity must be isolated, or the cell is shorted. That is the insulating adhesive, printed at cell level and cured before interconnection.

Both jobs went to ultraviolet cure for four reasons.

  • Speed. Cure takes seconds, matching stringer takt with no long oven behind the machine.
  • Temperature. Room-temperature cure adds no heat stress to wafers that keep getting thinner.
  • Cleanliness. One part, no solvent, nothing to mix and nothing to evaporate.
  • Control. Cure happens only where light lands, so the dispensing window is wide and a stopped line does not block a nozzle.

Supplier catalogs already list UV products for 0BB fixing, BC insulation, BC isolation, plating protection and perovskite encapsulation. This article stays on the two highest-volume jobs.

Four ingredients, two cure paths

A UV adhesive is four ingredients: an oligomer that forms the backbone, a reactive monomer that thins the viscosity and then reacts into the same network, a photoinitiator that absorbs ultraviolet light, and additives or fillers that tune adhesion, thixotropy and shelf life.

What separates the families is the cure path, and the cure path is where the failures come from.

Radical cure: fast, and inhibited by air

The photoinitiator splits under ultraviolet light into radicals that add across acrylate double bonds in a chain reaction. It is extremely fast. Oxygen consumes radicals too, so an exposed surface stays tacky while the bulk is hard. Linked double bonds sit closer together, so the part shrinks, commonly by 5% to 10%, and that stress works against adhesion. Switch the lamp off and the reaction stops.

Cationic cure: slow, and still running

An onium salt photoinitiator generates a strong acid on exposure, and the acid opens epoxy rings. Opening a ring does not pull molecules closer, so shrinkage stays near 2% to 4%. Oxygen does not interfere, which is why these surfaces come out dry. The acid keeps working in the dark after the lamp goes off. The costs are speed, and sensitivity to moisture and alkali.

Acrylate: the fastest way to pin a ribbon

A polyester acrylate or pure acrylate oligomer with acrylate monomers, cured by radicals. It is the most mature and highest-volume family in UV adhesives.

It is the fastest of the four, from under a second to a few seconds under high-irradiance LED. Viscosity, hardness and modulus adjust across a wide range. Clarity is high, aliphatic structures resist yellowing, the raw materials are mature and the cheapest of the four, and absorption matches the 365 to 405 nm LEDs that stringers use.

The costs are specific. Oxygen inhibition is worse in a thin layer, and a positioning bead is a thin layer. Shrinkage of 5% to 10% leaves stress at the interface. Adhesion to metal, glass and silicon nitride is only fair, so the formulation needs an adhesion-promoting monomer or a silane coupling agent. Ester bonds resist damp-heat hydrolysis only moderately, and anything the lamp cannot see stays uncured.

On a PV line this is the usual base for a 0BB positioning adhesive: nothing else cures inside the takt.

Cationic epoxy: the layer that cures after the lamp

This means cationic photocuring epoxy: alicyclic epoxy or oxetane with an iodonium or sulfonium salt. A different chemistry rather than a variation, so the trade-offs barely overlap with the acrylates.

Ring-opening keeps shrinkage near 2% to 4%. With no oxygen inhibition the surface comes out dry. Adhesion to metal, glass and ceramic is excellent, crosslink density is high, and hardness, heat resistance, chemical resistance and insulation follow from it. Dark reaction plus a bake pushes conversion further, which matters when a layer has to hold voltage for years.

It is slow and usually needs the bake. Humidity slows it. Amines, alkaline fillers and some substrates poison it. The cured film is brittle and needs toughening. Onium salts absorb weakly at 395 and 405 nm, so a sensitizer is normally required. Residual acid and ions are a corrosion risk on metallization, and the materials cost more.

The job follows: insulation, isolation and protection, wherever hardness, dielectric strength and chemical resistance outweigh seconds.

Epoxy acrylate: one name, two materials

Two different products are sold under this name, and the first question in a technical exchange should be which one the other side means.

Epoxy acrylate: an epoxy skeleton, a radical cure

An epoxy resin reacted with acrylic acid. The backbone is epoxy, usually bisphenol A, and the ends are acrylate double bonds, so the cure is still radical. It inherits hardness and chemical resistance, keeps acrylate speed, and is cheap. It is brittle, viscous, and the aromatic backbone yellows.

Hybrid: two initiators, one network

Acrylate and epoxy in one formulation with two initiators. Cured, they form an interpenetrating network: the acrylate sets the shape quickly, then the epoxy strengthens by dark reaction or heat. Shrinkage and adhesion land between the parents, and oxygen inhibition and moisture sensitivity partly cancel. The price is formulation complexity, storage stability and a narrower process window.

What you buy is speed with hardness, heat and chemical resistance, insulation, lower shrinkage than a pure acrylate, and an easy route to UV plus heat dual cure. What you pay is brittleness, yellowing on aromatic grades, and tighter process control.

On a PV line it is the common choice for a BC insulating adhesive, and for positioning adhesives that must finish curing in shadow.

Polyurethane acrylate: where the copper gap is paid

An isocyanate and a polyol make a polyurethane prepolymer, capped with a hydroxyl-bearing acrylate. Soft and hard segments alternate, the ends are acrylate double bonds, and the cure is radical.

Toughness and elongation are the best of the four, so thermal shock and fatigue are where it earns its place. Urethane bonds hydrogen bond to surfaces, which helps adhesion without promoters. It stays flexible when cold, aliphatic grades resist yellowing, and polyol type and molecular weight tune hardness almost continuously.

It is viscous, so it needs more diluent monomer. It cures slightly slower than epoxy acrylate, and its hardness and heat ceiling are lower. Polyether soft segments are weaker against heat, oxygen and ultraviolet light, polyester segments against hydrolysis, and polycarbonate segments are best and dearest. Aromatic grades yellow.

Here is where the architecture reaches the chemistry. Copper expands at about 17 ppm/K and silicon at about 2.6 ppm/K, more than six times apart, and the ribbon that carries that copper touches the cell directly. A fielded module cycles daily, so every dot is pulled back and forth daily, and a dot too hard and brittle cracks or debonds after thermal cycling. That is the work polyurethane acrylate is hired for.

ChemistryCharacter in one lineWhat to watchTypical job
AcrylateFastest, cheapest, widest adjustment rangeShrink stress, oxygen inhibition, shadow areas that never cure0BB positioning adhesive
Cationic epoxyLow shrink, strong adhesion, high insulationMoisture and alkali poisoning, brittleness, residual acidInsulation, isolation, protection
Epoxy acrylate, or hybridFast and hard, good chemical resistanceBrittleness, yellowing on aromatic gradesBC insulation adhesive, shadow-cured positioning
Polyurethane acrylateTough, tolerant of thermal cyclingHardness and heat ceiling, soft-segment aging0BB positioning, as toughener or base resin

Real products are almost never pure. A production positioning adhesive is often an acrylate monomer with polyurethane acrylate for toughness and a little epoxy acrylate for hardness. The family name says which one dominates, and so which failure you manage.

Two job descriptions that are nearly opposite

Written side by side, the two job descriptions come out close to inverses. No single formulation serves both well, which is why the materials split rather than converge.

The two UV adhesive jobs on a left panel, positioning on 0BB and isolation on BC, with four chemistries, their main risk and their usual job on a right panel

Left: the two jobs the new architectures created, one that pins a ribbon and one that isolates it. Right: four chemistries with the failure each is hired to prevent. Not to scale.

RequirementPositioning adhesive (0BB)Insulating adhesive (BC)
Cure speedSeconds, inside the stringer taktFast enough for high-speed screen printing
SurfaceDry, no blocking when strings stackDry, clean printed edges, no bleed
MechanicalPeel strength, tough through cyclingHard, not crushed during lamination
ElectricalNot the deciding propertyResistivity, withstand voltage, no pinholes
HeatNo flow at 140 to 160 °C in the laminatorShort excursion above 200 °C if soldered
YellowingHard specification, the dot sits in daylightLower priority, the rear sees little UV
Typical familyAcrylate with polyurethane acrylateEpoxy acrylate, hybrid, or thermal epoxy

A positioning adhesive is judged on speed, toughness and clarity: a dry surface so stacked strings do not block, a sub-millimeter dot with enough thixotropy not to string or slump, peel strength that survives 140 to 160 °C without flowing, no reaction with film additives or flux residue, and yellowing resistance as a hard spec.

During encapsulation, we hold platen temperatures strictly inside the 140 to 160 °C window so that cured positioning beads resist displacement and do not flow under vacuum before the encapsulant sheet sets.

An insulating adhesive is judged on the other axis: a layer a few tens of micrometers thick with no pinholes, high resistivity and withstand voltage, enough hardness not to be crushed when the ribbon presses down, survival of a short excursion above 200 °C if the interconnection is soldered, clean printed edges, and stability through damp heat, thermal cycling and PID.

To prevent crushing this layer of a few tens of micrometers, we regulate membrane pressure and chamber evacuation rates so the ribbon beds down without piercing the underlying dielectric during the heat cycle.

They agree on one thing: ionic cleanliness, and the film they will be laminated against.

A selection order, not a chemistry quiz

The order I would defend is job, then shadow, then yellowing and insulation, then cost. Family names come after that, as a consequence.

  • Job first. Positioning or insulating, because the two requirement sets are inverses.
  • Shadow second. A ribbon is opaque, so the adhesive beneath it receives no ultraviolet light. If the joint cannot tolerate an uncured underside, the answer is UV plus heat dual cure.
  • Yellowing and insulation third. A front-side dot needs aliphatic structures and a photoinitiator package that will not discolor. A rear-side layer needs dielectric strength and ionic cleanliness, and sees little light, so yellowing drops.
  • Cost last. The spread between families is small next to a failed qualification.
ApplicationFirst conflict to resolveCommon systems
0BB positioningFast, tough, yellowing-resistant, must not block lightAcrylate plus polyurethane acrylate; UV plus heat dual cure in shadow
BC insulationInsulating, hard, heat resistant, printableEpoxy acrylate or hybrid UV cure; thermal epoxy
BC isolation, plating protectionChemical resistance, dry surfaceEpoxy systems and their hybrids

Followed in that order, the route lands on the same three answers: acrylate with polyurethane acrylate for positioning, epoxy acrylate or a hybrid for BC insulation, epoxy systems for isolation and plating protection. None of those requires the full chemistry, which is the point.

Five ways material introduction goes wrong

Five things decide a material introduction, and none of them is a data sheet number.

  • Judging on initial adhesion. What matters is retention after damp heat and thermal cycling. A high initial peel says the adhesive worked the day it was applied, the one day nobody doubts.
  • Ignoring compatibility with the film. An adhesive that passes alone is not a laminate that passes, and the interface itself has its own article. The line-shaped bubbles along ribbons seen with EPE film are the same family of defect, arriving from the adhesive instead.
  • Not controlling the degree of cure. Monitor energy and irradiance, not one. LED aging and ribbon shadow cause undercure, and residual monomer then migrates or gases during lamination.
  • Letting dot volume and placement drift. Overflow onto a finger raises contact resistance, and on a 0BB dispensing line that is a common source of dark spots in electroluminescence.
  • Ignoring ions and acid value. Residual acid in a cationic system and acidic adhesion promoters in an acrylate both attack metallization, and the check is damp heat under bias. Ion content and acid value have to be low, and the cured adhesive must not corrode the silver or the copper fingers.

Where these numbers come from

The shrinkage ranges, cure times, finger width, expansion coefficients and the 140 to 160 °C window are typical magnitudes from public literature and supplier technical data, illustrative rather than measured on one product. Family comparisons are qualitative: the tendency of a chemistry, not the performance of a grade. Standard test names appear by name only, without clause numbers, because what is quoted here are ranges. We measured no stack, name no suppliers and quote no prices. Where a number looks precise, read it as a specification starting point, not as company test data.

Frequently asked questions

Q: Does every 0BB interconnect route need an adhesive?

No. Three routes are discussed in public: dispensing with UV cure, soldering followed by dispensing, and a carrier or skin film such as IFC that holds the ribbon dry. Two of the three use adhesive.

Q: Can one adhesive serve the positioning and the insulating job?

Not well. One is asked to be fast, tough and clear, the other hard, void-free and insulating, and a formulation that maximizes one gives up the other. They also sit on different faces, with different light budgets.

Q: Why not use thermal-cure epoxy everywhere and skip the lamp?

It costs takt, it puts heat into wafers that are already thin, and a positioning dot has to hold before the string moves at all. Thermal epoxy stays safer where insulation margin beats seconds.

Q: Which chemistry should a BC insulating layer use?

Epoxy acrylate or a radical-cationic hybrid if the layer is printed and UV cured, because both give hardness and insulation at printing speed. Thermal epoxy remains the option when heat and dielectric margin carry more weight.

Q: Does an acrylate always yellow?

The backbone decides more than the family name. Aliphatic structures hold color better than aromatic ones, and a front-side dot lives in daylight, so grade and photoinitiator package matter more than the word on the drum.

Q: What does a supplier mean by epoxy acrylate?

Ask which of two things. Epoxy acrylate is an epoxy backbone with acrylate ends and still cures by radicals. A radical-cationic hybrid contains both chemistries and two initiators. The name alone is not a specification.

Q: Does a thicker insulating layer insulate better?

Not as much as it looks. The layer is already only tens of micrometers, pinholes and voids are the failure path rather than bulk thickness, and a thicker layer is harder to cure at depth and easier to crush in lamination.

Q: Where does dual cure earn its cost?

Under the ribbon, which is opaque, and in thick or shadowed geometry. The UV step sets the dot so the string can be handled, and the heat of lamination finishes the conversion where light never arrived.

Final thoughts

Acrylate wins on speed, epoxy on stability, epoxy acrylate on speed with hardness, polyurethane acrylate on toughness. Those four sentences only help after the job is written down, because the two jobs in a 0BB or BC module pull in opposite directions. Write the job first, decide whether the lamp reaches everywhere, and the family mostly chooses itself.

OOITech manufactures oil-heated and electric solar panel laminator machines in single and double chamber configurations to support precise curing profiles. Send us your module stack, string layout drawings, or test samples so our engineering team can evaluate thermal performance and pressure distribution for your adhesive system.


Tags :

Request A Quote

All uploads are secure and confidential.

Type the characters shown in the image beside this field.
Verification code image, click to refresh
Why Choose Us

We deliver expertise you can trust our service

Direct-from-Factory Equipment.

Cost-Effective Advantages

We deliver exceptional value, maximizing results while optimizing budgets for clients.

Our Experience Team

Our skilled professionals specialize in innovative solutions and tailored strategies.

15+ Years Industry Experience

Deep expertise ensures reliable, trend-aware, and proven outcomes for success.

Testimonials

What Our Client Say's about us

Client testimonials praise our deep understanding of their challenges, which leads to innovative solutions and strong ROI. Long-term collaborations—some over a decade—demonstrate their trust and satisfaction. Their success stories drive us to continually exceed expectations. Know More

Our Products

Our Latest Products

PV Ribbon Production Line: Drawing, Rolling, Tinning
2026-05-11 16:28:19

PV Ribbon Production Line: Drawing, Rolling, Tinning

Professional integrated PV busbar ribbon production line combining wire drawing, rolling, flat drawing, annealing and tin coating processes for high

Read More
SC-20D Dual-Laser Solar Cell Cutting Machine
2025-08-17 17:41:21

SC-20D Dual-Laser Solar Cell Cutting Machine

SC-20D is the advanced version of SC-20A, specially designed for shingled solar cell production, featuring dual laser heads and two lasers working

Read More
CHT9980A PV Safety Tester: 8kV, 0.001kV Resolution
2025-09-08 13:59:50

CHT9980A PV Safety Tester: 8kV, 0.001kV Resolution

CHT9980A/CHT9981A PV Safety Comprehensive Tester is a high-performance 3-in-1 instrument integrating DC withstand voltage, insulation resistance

Read More
Solar Cells for PV Modules
2025-09-09 09:29:14

Solar Cells for PV Modules

Solar cell processing equipment for PERC, TOPCon, HJT & BC cells – cutting, stringing, testing. Supports G1/M6/M10/M12 sizes.

Read More
Low-Temperature PV Ribbon and Flux for Solar Strings
2025-09-10 08:55:26

Low-Temperature PV Ribbon and Flux for Solar Strings

PV ribbon and flux for solar cell interconnection: low-temperature soldering ribbon in high-purity tin-coated copper, supporting MBB and half-cut lines.

Read More
Full Automatic Solar Panel Production Line Equipment
2025-09-06 11:32:53

Full Automatic Solar Panel Production Line Equipment

Ooitech full automatic solar panel production line covers glass loading, EVA laying, string layout, tape sticking, lamination, trimming, framing

Read More
AI research shortcut

Ask AI About OOITech

One click opens your AI assistant with a question about our solar panel production lines already filled in — the turnkey PV module lines we build, from semi-automatic to GW-scale, and what a quote needs.

Get a Quote